Same drum, two ends of the day.
The first stretch of film in the morning sits on the plus side of the thickness window.
By afternoon the whole roll has dropped to the minus side.
Nothing on the pump, nothing on the gap, not one number changed on the setup sheet.
Walk over to the slurry drum and look in.
A thin layer floats on top, and what you scrape off the bottom stirs only after a couple of turns of the agitator.
The viscometer read twenty-five hundred yesterday. The same drum reads eighteen hundred today.
Weigh one cup from the top and one from the bottom, and the solids up top sit nearly ten percent lower.
Every sign points the same way. The slurry has split itself apart while standing.
Why does a slurry settle, where do the coarse particles go, and is there anything left to save before the pump starts?
1. Size and Density Set the Pace
The pace follows an equation, and the stokes one is enough here. Take a ten micron particle with a density gap of two grams per cubic centimetre. In a slurry at one thousand mPa·s it drops roughly a centimetre a day. Double the size and the pace goes up fourfold.
Why do the coarse ones go first?
Drag grows with the square of the size. The fraction under two microns rides along with the slurry and takes no part in the layering.
The drum never settles as one body.
No matter how even the D50 looks, it does not govern the D99 tail. The coarse grades move first and pack together at the bottom. The tail of the distribution tells you more than the average does.
More than one supplier reports only the average on that table. The D99 is yours to ask for.
2. Cut the Viscosity and Settling Speeds Up
Thinning is the usual pusher, and settling speed runs inverse to viscosity. A slurry at one thousand mPa·s drops a centimetre a day. Thin it to five hundred and the same particle walks four centimetres a day. You thin the batch so it coats better. It flows nicely for the moment, and settling speeds up in the drum and in the tank at the same time.
The line sits overnight, and you thin it again next morning. After two or three rounds the bottom of the drum starts to cake.
Rheology additives have a real job here. A small thixotropic structure lets the slurry hold itself up at rest and thin out under shear. On the rheology curve from the slurry supplier, look for a thixotropic loop.
A flat curve means the slurry cannot carry itself, and the tank has to hold it up instead.
3. The Drum Settles Before the Tank Does
The drum is the first station, and the feed tank is only the second. Powder and resin differ in density by nature. A drum left over the weekend stands with a concentration gradient inside.
Draw straight from the drum and the first stretch runs lean while the last runs rich. Coat weight walks a slope within the batch.
Roll the drum for twenty minutes before you pour. It costs you little and saves half the drift inside a batch.
The day you skip it, the thickness is walking that slope.
The roller rack ships with the line, sits on the packing list of the machine builder, and where it is missing you ask. Inside the tank the logic repeats.
A tank drawn down through the afternoon gives up its rich bottom last. Viscosity climbs as the level falls, and the final stretch goes erratic.
4. Where the Tank Hides Its Dead Zones
The tank has a share too, for the corners of a flat bottom hold still. Coarse particles settle in the corners and in the ring the agitator cannot reach. A few weeks later it is a hard cake that needs chipping out.
A sloped or conical bottom leads the slurry to the outlet, and the impeller sits low and true. The return line enters below the liquid surface, so the stream does not hammer air into the batch.
All of this belongs on the tank drawing, and the machine builder sets it there. A coating line manufacturer puts circulation volume and residence time into the proposal, and commissioning checks against it.
Low points in the piping hold slurry too. Stop the pump and coarse particles sit down at the low spots. The next start-up carries them into the head, and the first metre of film shows every one.
Drain valves go at the low points, the positions marked on the machine builder's drawing. That section gets flushed before shutdown.
The slurry sitting in that low corner, who is going to flush it out for you?
Ask for it at handover and it will not slip out of the training.
5. Two Numbers Pin Settling Down
Judgement can skip the film. A cup left standing half an hour shows a layer line against the light. Weighing solids has a routine of its own, called the oven method. Tare the dish and take two grams, bake at one hundred and five degrees to a constant weight, and the difference is the solids.
Disputes between the two sides of a delivery are settled by the same figure. One cup from the top of the drum, one from the bottom.
What does a gap above two percent mean?
It means the drum needs handling before it goes on the machine.
Take the gap between the two cups to a coating machine manufacturer. The question of residence time and circulation margin then gets a straight answer. Record one thickness for the first article and one for the tail. The slope between them is the path settling walked through the batch.
The words "just stir it even" do not survive contact with settling.
Pick the remedy by the source.
A layered drum goes on the roller rack and gets used straight after rolling, not left overnight. A tank with settled slurry goes on circulation, one pass per shift.
The soft layer stirs back in, and the hard cake does not. Can it be stirred back? No, and that is why tank cleaning sits in the maintenance plan with its hours and its downtime.
A coating line supplier lists tank cleaning as its own line item, so you know what the account looks like before you sign.
Where the cause sits in the formula, go back to rheology and size control. Sit the slurry supplier and the equipment supplier down with one curve between them.
The trial report should carry a standing test. Where the equipment supplier has not run one, have it run before you sign.
Where an OEM coordinates the project, write the boundary for settling down. Layering in the drum belongs to the formula, a cake in the tank belongs to the tank.
A manufacturer who has run your kind of powder can say how far the solids separate in twenty-four hours of standing. The figure goes into the minutes by the OEM's coordinator.
When settling returns within a batch, have a coating line supplier check the circulation volume. The number a coating line manufacturer recorded at commissioning is the standard to compare against later.
Three items belong on paper.
The drift limit for solids over standing time.
The agitation and circulation method of the feed tank.
The rolling requirement before a drum goes on the machine.
Check the proposal from a coating machine manufacturer against those three, line by line. When settling keeps coming back on site, have a coating machine manufacturer judge whether the tank or the slurry is at fault.
Settling scatters across size, viscosity and residence time. In the end the requirements come down to how rheology data, tank geometry and daily handling fit together.
Problems like this come up often in custom work. Innater works precision, thickness and uniformity out against your slurry's settling behaviour, machine by machine.
Write the solids drift limit and the drum rolling requirement into the technical agreement. The hard cake at the bottom of the drum is the receipt for what the agreement left out.

Multifunctional Coating Machine-Innate

Resist Coating-Innate
Published by Innater Intelligent Equipment Co., Ltd, a maker of non-standard coating machines and automated lines. Email 13316631159@163.com | Website https://www.getinnater.com/ | Tel +8613316631159